FeO
CaO
Cr2O3
MnO
NiO
�@
Fe2O4
CoO
�@

Ž_‰»•¨Œ‹�»
KTaO3 (Potassium Tantalate Single Crystals)
ƒ^ƒ“ƒ^ƒ‹Ž_ƒJƒŠƒEƒ€’PŒ‹�»

“Á�«�F

•ªŽq—Ê

268.04

�ƒ“x

99.99%

Œ‹�»�\‘¢

—§•û�», ƒyƒ�ƒuƒXƒJƒCƒg�\‘¢

ŠiŽq’è�”

a = 3.989 �ð 

–§“x

7015 g / cc

”M“`“±—¦

0.17 w/m.k at 300k

‹ü�Ü—¦

2.14

ƒZƒ‹ƒ}ƒCƒ„•û’öŽ®

ho2 -1 =3.591ƒÉ2 / (ƒÉ2 -(0.193) 2 )  
(ƒÉin ƒÊm, from 0.4 - 1.06 ƒÊm )

ˆç�¬•û–@

Top seed flux growth

•W�€Žd—l�F

•W�€ƒTƒCƒY

10 mm x 10 mm x 0.5 mm                 

–Ê•ûˆÊ

(100) , (110)

޲�¸“x

+ / - 0.5�‹

Œ¤–�

•Жʖ”‚Í—¼–ÊŒ¤–�

•\–Ê‘e‚³

< 10 �ð

KTaO3’PŒ‹�»

‚¨–â‚¢�‡‚킹 Дޮ‰ïŽÐƒlƒIƒgƒ�ƒ“